Al-GMAW - straight run or whipping motion?

<lybl6w2odi.fsf@richards-air-2.home>

  copy mid

https://www.novabbs.com/tech/article-flat.php?id=70&group=sci.engr.joining.welding#70

  copy link   Newsgroups: sci.engr.joining.welding
Path: i2pn2.org!i2pn.org!aioe.org!LQ49Ht18l52J+4ZKZzm2Gw.user.46.165.242.91.POSTED!not-for-mail
From: nul...@void.com (Richard Smith)
Newsgroups: sci.engr.joining.welding
Subject: Al-GMAW - straight run or whipping motion?
Date: Wed, 21 Jul 2021 07:05:13 +0100
Organization: Aioe.org NNTP Server
Message-ID: <lybl6w2odi.fsf@richards-air-2.home>
Mime-Version: 1.0
Content-Type: text/plain; charset=us-ascii
Injection-Info: gioia.aioe.org; logging-data="17061"; posting-host="LQ49Ht18l52J+4ZKZzm2Gw.user.gioia.aioe.org"; mail-complaints-to="abuse@aioe.org";
User-Agent: Gnus/5.11 (Gnus v5.11) Emacs/22.1 (darwin)
X-Notice: Filtered by postfilter v. 0.9.2
Cancel-Lock: sha1:4Zj9MGlSpq18eHYWBjFPxXDLwUY=
 by: Richard Smith - Wed, 21 Jul 2021 06:05 UTC

Hi again

Al-GMAW

Some say - straight run
Others say - weave or "whip"

You say??

Rich S

Re: Al-GMAW - straight run or whipping motion?

<sd9h1i$g7s$1@dont-email.me>

  copy mid

https://www.novabbs.com/tech/article-flat.php?id=71&group=sci.engr.joining.welding#71

  copy link   Newsgroups: sci.engr.joining.welding
Path: i2pn2.org!i2pn.org!eternal-september.org!reader02.eternal-september.org!.POSTED!not-for-mail
From: muratla...@gmail.com (Jim Wilkins)
Newsgroups: sci.engr.joining.welding
Subject: Re: Al-GMAW - straight run or whipping motion?
Date: Wed, 21 Jul 2021 12:12:24 -0400
Organization: A noiseless patient Spider
Lines: 1
Message-ID: <sd9h1i$g7s$1@dont-email.me>
References: <lybl6w2odi.fsf@richards-air-2.home>
Mime-Version: 1.0
Content-Type: text/plain;
format=flowed;
charset="iso-8859-1";
reply-type=original
Content-Transfer-Encoding: 7bit
Injection-Date: Wed, 21 Jul 2021 16:12:34 -0000 (UTC)
Injection-Info: reader02.eternal-september.org; posting-host="7129edc2147884e21ab855feec584617";
logging-data="16636"; mail-complaints-to="abuse@eternal-september.org"; posting-account="U2FsdGVkX1+JC5W3TwPEaygyImCqnnJGmLOwGxWHZTc="
Cancel-Lock: sha1:ZmgffZ1XinxQLOjDTU5adDZZ3Qo=
X-MimeOLE: Produced By Microsoft MimeOLE V16.4.3505.912
In-Reply-To: <lybl6w2odi.fsf@richards-air-2.home>
X-Antivirus-Status: Clean
X-Newsreader: Microsoft Windows Live Mail 16.4.3505.912
Importance: Normal
X-Antivirus: AVG (VPS 210721-4, 07/21/2021), Outbound message
X-Priority: 3
X-MSMail-Priority: Normal
 by: Jim Wilkins - Wed, 21 Jul 2021 16:12 UTC

"Richard Smith" wrote in message news:lybl6w2odi.fsf@richards-air-2.home...

Hi again

Al-GMAW

Some say - straight run
Others say - weave or "whip"

You say??

Rich S

--------------------

https://www.mig-welding.co.uk/forum/

Re: Al-GMAW - straight run or whipping motion?

<lyr1fqozgd.fsf@richards-air-2.home>

  copy mid

https://www.novabbs.com/tech/article-flat.php?id=72&group=sci.engr.joining.welding#72

  copy link   Newsgroups: sci.engr.joining.welding
Path: i2pn2.org!i2pn.org!aioe.org!LQ49Ht18l52J+4ZKZzm2Gw.user.46.165.242.91.POSTED!not-for-mail
From: nul...@void.com (Richard Smith)
Newsgroups: sci.engr.joining.welding
Subject: Re: Al-GMAW - straight run or whipping motion?
Date: Thu, 22 Jul 2021 21:39:30 +0100
Organization: Aioe.org NNTP Server
Message-ID: <lyr1fqozgd.fsf@richards-air-2.home>
References: <lybl6w2odi.fsf@richards-air-2.home> <sd9h1i$g7s$1@dont-email.me>
Mime-Version: 1.0
Content-Type: text/plain; charset=us-ascii
Injection-Info: gioia.aioe.org; logging-data="16069"; posting-host="LQ49Ht18l52J+4ZKZzm2Gw.user.gioia.aioe.org"; mail-complaints-to="abuse@aioe.org";
User-Agent: Gnus/5.11 (Gnus v5.11) Emacs/22.1 (darwin)
Cancel-Lock: sha1:KLX3oQRGH8H2lKzWcrs0HVrO7do=
X-Notice: Filtered by postfilter v. 0.9.2
 by: Richard Smith - Thu, 22 Jul 2021 20:39 UTC

"Jim Wilkins" <muratlanne@gmail.com> writes:

> "Richard Smith" wrote in message news:lybl6w2odi.fsf@richards-air-2.home...
>
> Hi again
>
> Al-GMAW
>
> Some say - straight run
> Others say - weave or "whip"
>
> You say??
>
> Rich S
>
> --------------------
>
> https://www.mig-welding.co.uk/forum/

Latest - running smoothly
5083 Al plate 6mm thickness
5356 GMAW wire 1.2mm (47thou") diameter
in spray at
9.8m/min
(385"/min)
and about 22.8V reported.
Smooth run, no manipulation.
Looks good. Is good?

Only remaining problem is the restarts. Often burn-back to the torch
/ contactor tip. Blob of Al against contactor tip which prizes off
without harm if quick off the trigger.
Not yet worked out how to avoid that.

If I could solve that, I'd be doing rather well.
No other problems remaining

I'm left totally puzzled why Pulse is used on this 6mm thickness when
you'd be a "clean" spray anyway...

In spray doing overhead - 4F/PD - no metal ejection, not getting
burned.
Basis to insist on CV spray, as getting covered in burns using Pulse,
which was ejecting a drop of spatter per pulse.

Now finding every other position good.

I was worried the weld beads are too smooth suggesting excessive heat
input - but
- am on only about 210A to 220A (Linc.Elec. A for 9.8m/min with
1.2mm-dia wire) at just under 23V - low-end of L.E. volts range.
- any drop in V by a tiny amount or wire-feed-speed / Amps causes a
coarse unwetted bead and raspy arc - only just in spray
indicate the concern is misplaced - the beads are smooth and that is
the way it is not problem (the reference state being Pulse welded bead
appearance)

Rich S