tech / sci.engr.joining.welding / Re: Al-GMAW - restarts without burnback

SubjectAuthor
* Al-GMAW - restarts without burnbackRichard Smith
+- Re: Al-GMAW - restarts without burnbackJim Wilkins
`* Re: Al-GMAW - restarts without burnbackBob La Londe
 `- Re: Al-GMAW - restarts without burnbackRichard Smith

1
Al-GMAW - restarts without burnback

<lya6mdy40h.fsf@richards-air-2.home>

  copy mid

https://www.novabbs.com/tech/article-flat.php?id=73&group=sci.engr.joining.welding#73

  copy link   Newsgroups: sci.engr.joining.welding
Path: i2pn2.org!i2pn.org!weretis.net!feeder8.news.weretis.net!news.mixmin.net!aioe.org!LQ49Ht18l52J+4ZKZzm2Gw.user.46.165.242.91.POSTED!not-for-mail
From: nul...@void.com (Richard Smith)
Newsgroups: sci.engr.joining.welding
Subject: Al-GMAW - restarts without burnback
Date: Fri, 23 Jul 2021 06:48:30 +0100
Organization: Aioe.org NNTP Server
Message-ID: <lya6mdy40h.fsf@richards-air-2.home>
Mime-Version: 1.0
Content-Type: text/plain; charset=us-ascii
Injection-Info: gioia.aioe.org; logging-data="40374"; posting-host="LQ49Ht18l52J+4ZKZzm2Gw.user.gioia.aioe.org"; mail-complaints-to="abuse@aioe.org";
User-Agent: Gnus/5.11 (Gnus v5.11) Emacs/22.1 (darwin)
X-Notice: Filtered by postfilter v. 0.9.2
Cancel-Lock: sha1:KFG/bMbgCF8HsOdR1sQ/0fRvjoc=
 by: Richard Smith - Fri, 23 Jul 2021 05:48 UTC

Hi all

Burn-back to contactor tip on pulling trigger is my big problem at the
moment.

Wire feed is smooth.
I clean out the contactor-tip frequently with an oxy-acetylene nozzle
cleaner - the set of serated wires.

Yet - often - very quickly - burns back in fraction of a second so
arc'ing off a blob on the contactor tip.

I'm trying things like holding a greater stand-off on start-up.

Will try snipping off wire at shroud so wire-feed has time to come up
to speed (?) before wire touches job.

Etc.

Hints?

Best wishes,
Rich Smith

Re: Al-GMAW - restarts without burnback

<sde6gh$jmb$1@dont-email.me>

  copy mid

https://www.novabbs.com/tech/article-flat.php?id=74&group=sci.engr.joining.welding#74

  copy link   Newsgroups: sci.engr.joining.welding
Path: i2pn2.org!i2pn.org!eternal-september.org!reader02.eternal-september.org!.POSTED!not-for-mail
From: muratla...@gmail.com (Jim Wilkins)
Newsgroups: sci.engr.joining.welding
Subject: Re: Al-GMAW - restarts without burnback
Date: Fri, 23 Jul 2021 06:43:19 -0400
Organization: A noiseless patient Spider
Lines: 1
Message-ID: <sde6gh$jmb$1@dont-email.me>
References: <lya6mdy40h.fsf@richards-air-2.home>
Mime-Version: 1.0
Content-Type: text/plain;
format=flowed;
charset="iso-8859-1";
reply-type=original
Content-Transfer-Encoding: 7bit
Injection-Date: Fri, 23 Jul 2021 10:43:29 -0000 (UTC)
Injection-Info: reader02.eternal-september.org; posting-host="7c12b9c23cd823564580da459ff7fa53";
logging-data="20171"; mail-complaints-to="abuse@eternal-september.org"; posting-account="U2FsdGVkX1/v5QNLMXGhcSlpc2Z/FYt3vrQuBNg4dJM="
Cancel-Lock: sha1:64PrmF+nXkZS7Y0ItXjmglDkYLQ=
X-MimeOLE: Produced By Microsoft MimeOLE V16.4.3505.912
In-Reply-To: <lya6mdy40h.fsf@richards-air-2.home>
X-Antivirus-Status: Clean
X-Newsreader: Microsoft Windows Live Mail 16.4.3505.912
Importance: Normal
X-Antivirus: AVG (VPS 210723-0, 07/22/2021), Outbound message
X-Priority: 3
X-MSMail-Priority: Normal
 by: Jim Wilkins - Fri, 23 Jul 2021 10:43 UTC

"Richard Smith" wrote in message news:lya6mdy40h.fsf@richards-air-2.home...

Hi all

Burn-back to contactor tip on pulling trigger is my big problem at the
moment.

Wire feed is smooth.
I clean out the contactor-tip frequently with an oxy-acetylene nozzle
cleaner - the set of serated wires.

Yet - often - very quickly - burns back in fraction of a second so
arc'ing off a blob on the contactor tip.

I'm trying things like holding a greater stand-off on start-up.

Will try snipping off wire at shroud so wire-feed has time to come up
to speed (?) before wire touches job.

Etc.

Hints?

Best wishes,
Rich Smith

---------------------

https://americantorchtip.com/blog/5-causes-of-contact-tip-burnback/

Re: Al-GMAW - restarts without burnback

<sdeu4n$19ic$1@gioia.aioe.org>

  copy mid

https://www.novabbs.com/tech/article-flat.php?id=75&group=sci.engr.joining.welding#75

  copy link   Newsgroups: sci.engr.joining.welding
Path: i2pn2.org!i2pn.org!aioe.org!8O4CTVvGI43OLyHlA+QjDA.user.46.165.242.75.POSTED!not-for-mail
From: non...@none.com99 (Bob La Londe)
Newsgroups: sci.engr.joining.welding
Subject: Re: Al-GMAW - restarts without burnback
Date: Fri, 23 Jul 2021 10:26:46 -0700
Organization: Aioe.org NNTP Server
Message-ID: <sdeu4n$19ic$1@gioia.aioe.org>
References: <lya6mdy40h.fsf@richards-air-2.home>
Mime-Version: 1.0
Content-Type: text/plain; charset=utf-8; format=flowed
Content-Transfer-Encoding: 7bit
Injection-Info: gioia.aioe.org; logging-data="42572"; posting-host="8O4CTVvGI43OLyHlA+QjDA.user.gioia.aioe.org"; mail-complaints-to="abuse@aioe.org";
User-Agent: Mozilla/5.0 (Windows NT 10.0; Win64; x64; rv:78.0) Gecko/20100101
Thunderbird/78.12.0
Content-Language: en-US
X-Antivirus: AVG (VPS 210723-8, 7/23/2021), Outbound message
X-Antivirus-Status: Clean
X-Notice: Filtered by postfilter v. 0.9.2
 by: Bob La Londe - Fri, 23 Jul 2021 17:26 UTC

On 7/22/2021 10:48 PM, Richard Smith wrote:
> Hi all
>
> Burn-back to contactor tip on pulling trigger is my big problem at the
> moment.
>
> Wire feed is smooth.
> I clean out the contactor-tip frequently with an oxy-acetylene nozzle
> cleaner - the set of serated wires.
>
> Yet - often - very quickly - burns back in fraction of a second so
> arc'ing off a blob on the contactor tip.
>
> I'm trying things like holding a greater stand-off on start-up.
>
> Will try snipping off wire at shroud so wire-feed has time to come up
> to speed (?) before wire touches job.
>
> Etc.
>
> Hints?
>
> Best wishes,
> Rich Smith
>

I'm absolutely not an expert or even a good apprentice at any kind of
welding, however your experience mirrors mine in the few dozen feet of
aluminum bead I have laid down with a spool gun. There are a couple
little tricks that helped.

* 3/4 inch stickout. Yes, really. That much.

* Shorten the inner tube the contact tip screws into. I shortened the
inner tube about 3/16 inch and threaded it deeper for the tips. This
helps you maintain stick out.

* Clip the bead off the end of the wire every single time I stop. I
found if I had a ball on the end of the wire burn back was much worse
than if I clipped it off every single time.

* Some sort of gas lens inside the nozzle to better unify the gas flow.
One youtube welder (I don't recall who) used some sort of very porous
scrubber material. I use a piece of screen.

* Don't trust the table on the flip card on the welder. (On my 212 I
almost universally needed slightly higher wire feed rate.) The flip
card values are only good for a starting point before making some
practice welds.

* Buy bulk tips off of your domestic import seller platform like Ebay,
and don't be afraid to swap them out and throw them away many times in a
modest large job.

* Don't be afraid to adjust the gas flow away from that suggested on
the tables. I haven't really needed to do this, but your mileage may vary.

* Look up information on line for travel speed and try to do a couple
cold runs at what you think is that travel speed for practice.

* if possible always make a hot practice weld or two on the same size
material as the job you will be doing. If you can make the practice
weld push it to the point of failure (usually drop out) so you know when
to stop, and always stop in half that time or bead length in your real
weld.

* Tack and fill switch areas allowing heat dissapation between short
welds if needed.

* Start and finish on a previous weld or tack.

* It might be possible to weld larger than 1/4 inch (6.35mm), but it
takes lots of preheat and maybe some non approved wallowing around with
the gun.

* Remember that while aluminum dissipates heat fast (problem with thick
stuff) it doesn't necessarily dissipate it as fast as you are putting it
in to a local area (problem with thinner stuff).

These things allow me to almost (but not always) make barely ok aluminum
welds even with my low hours on the gun. An experienced welder such as
yourself should be able to do better.

I have welded upto 3/8, but it was bad and took lots of work and
preheat. I found 1/8-1/4 was pretty easy to accomplish with down to .08
being within the capability of the machine if not necessarily within my
skill level. I did actually make one (1) very very short weld on .043
wall tube that was ok, but I had to whip the gun around the joint almost
as fast as I could move it.

These are ignorant beginner suggestions based on my limited experience.
Nearly all of them were learned from other welders on this group.

--
This email has been checked for viruses by AVG.
https://www.avg.com

Re: Al-GMAW - restarts without burnback

<lyczr8stc2.fsf@void.com>

  copy mid

https://www.novabbs.com/tech/article-flat.php?id=82&group=sci.engr.joining.welding#82

  copy link   Newsgroups: sci.engr.joining.welding
Path: i2pn2.org!i2pn.org!aioe.org!LQ49Ht18l52J+4ZKZzm2Gw.user.46.165.242.91.POSTED!not-for-mail
From: nul...@void.com (Richard Smith)
Newsgroups: sci.engr.joining.welding
Subject: Re: Al-GMAW - restarts without burnback
Date: Fri, 23 Jul 2021 20:50:21 +0100
Organization: Aioe.org NNTP Server
Message-ID: <lyczr8stc2.fsf@void.com>
References: <lya6mdy40h.fsf@richards-air-2.home> <sdeu4n$19ic$1@gioia.aioe.org>
Mime-Version: 1.0
Content-Type: text/plain; charset=us-ascii
Injection-Info: gioia.aioe.org; logging-data="30120"; posting-host="LQ49Ht18l52J+4ZKZzm2Gw.user.gioia.aioe.org"; mail-complaints-to="abuse@aioe.org";
User-Agent: Gnus/5.11 (Gnus v5.11) Emacs/22.1 (darwin)
X-Notice: Filtered by postfilter v. 0.9.2
Cancel-Lock: sha1:QqfZWYeZTvjOU2f895PdsTU6DQc=
 by: Richard Smith - Fri, 23 Jul 2021 19:50 UTC

Thanks for suggestions, respondents.

On topic of avoiding burn-back to contactor tip when trying to start
weld on Ali GMAW / MIG.

Stand-off - there is a spray shroud for the common industrial GMAW
guns.
On steel it makes a significant difference in the favourable
direction. On steel it also works well when using Pulse to get
spray-like characteristics on average Amps less than spray (as you
might do positionally welding on thinner material)
Must try one on Ali GMAW.
So that's
* keeping close in for good shielding
* having plenty of electrical stick-out (workpiece to contactor tip)

Contactor tips - even with regular cleaning, you get through a lot,
yes.

In all other ways, with being a commercial welder, and with having
good kit - all Miller industrial grade running off 3-phase supply -
when arc is running, get the welds I want, now.
It seems instinctive.
I suspect I may be able to make smaller faster welds in future - don't
need much fillet-size for joining a stiffener rib to a plate it is
stiffening - but don't want to try to run before can walk...


tech / sci.engr.joining.welding / Re: Al-GMAW - restarts without burnback

1
server_pubkey.txt

rocksolid light 0.9.81
clearnet tor